Colour fastness to washing and rubbing: causes of failure and technical solutions
Prepared by the SDLABCOMO S.r.l. technical team · Published on · 6 min read
Share on LinkedInColour fastness tests to washing (ISO 105-C06) and rubbing (ISO 105-X12) are among those most frequently required by specifications. A poor result means garments that bleed in the washing machine or stain other fabrics and skin.
Interpreting the results
Results are expressed using the grey scale from 1 (very poor) to 5 (excellent), both for change in the sample's colour and staining of adjacent fabrics. Most specifications require ratings between 3 and 4.
Washing: why it fails
Typical causes
- Incomplete dye fixation due to unsuitable dyeing times, temperatures or pH.
- Insufficient rinsing after dyeing, leaving residual hydrolysed dye.
- Selection of a dye class unsuitable for the fibre or the required fastness level.
Solutions
- Optimise the dyeing cycle and post-dyeing washing (soaping).
- Assess a fixing agent compatible with the required handle and light fastness.
- Repeat the test on a pilot batch before production.
Rubbing: why it fails
Wet rubbing is almost always more critical than dry rubbing. Dark shades, indigo and surface pigments are the most frequent cases.
- Dye or pigment remaining on the surface rather than penetrating the fibre.
- Printing binder that has not cured correctly.
- Finishes that reduce friction may improve dry rubbing fastness but do not resolve wet rubbing problems.
In summary
A fastness failure almost always has an identifiable process-related cause. Testing the sample and pilot batch using a standardised method makes it possible to correct the problem before it reaches the end customer.
Sources and references
Related test sheet: Colour fastness testing to washing, rubbing, perspiration and light